• Required reading for all forum users!!!

    Welcome!
    Register to access the full functionality of the GSResources forum. Until you register and activate your account you will not have full forum access, nor will you be able to post or reply to messages.

    A note to new registrants...
    All new forum registrations must be activated via email before you have full access to the forum.

    A Special Note about Email accounts!
    DO NOT SIGN UP USING hotmail, outlook, gmx, sbcglobal, att, bellsouth or email.com. They delete our forum signup emails.

    A note to old forum members...
    I receive numerous requests from people who can no longer log in because their accounts were deleted. As mentioned in the forum FAQ, user accounts are deleted if you haven't logged in for the past 6 months. If you can't log in, then create a new forum account. If you don't get an error message, then check your email account for an activation message. If you get a message stating that the email address is already in use, then your account still exists so follow the instructions in the forum FAQ for resetting your password.

    Have you forgotten your password or have a new email address? Then read the forum FAQ for details on how to reset it.

    Any email requests for "can't log in anymore" problems or "lost my password" problems will be deleted. Read the forum FAQ and follow the instructions there - that's what we have one for...

  • Returning Visitors

    If you are a returning visitor who never received your confirmation email, then odds are your email provider is blockinig emails from our server. The only thing that can be done to get around this is you will have to try creating another forum account using an email address from another domain.

    If you are a returning visitor to the forum and can't log in using your old forum name and password but used to be able to then chances are your account is deleted. Purges of the databases are done regularly. You will have to create a new forum account and you should be all set.

Preventing flash rust...

rustybronco

Forum Guru
Past Site Supporter
TGSR Superstar
Past Bard Award Winner
http://www.eng-tips.com/viewthread.cfm?qid=324397


Another treasure trove of digestible reading material...

I was responsible for the manufacture of M42 high speed steel at Crucible Materials Corporation for 10 years, and handled many different types of customer complaints and application issues. I never had a customer complain about corrosion issues with this grade, either during manufacturing or in application. This makes me wonder if you are exposing the material to chlorine during the manufacturing process. Are you mixing your own cutting fluids? Are you using city water for this purpose? During the summer months, municipalities often spike their water supplies with chlorine in order to kill bacteria that can otherwsie grow and spread disease. If you don't actively filter this excess chlorine out of the water (using charcoal filtration for example) before using it to mix your cutting fluids for machining, it will expose the M42 to a known corrosion agent.

Maui

Hebe7671

Ok, I did a few trial runs of washing the parts in DI water afrer the machining operations and found that it greatly reduced, but did not completly eliminate, the corrosion issue. With the DI water, there was no flash rust but after a few hours a few small spots of rust could be seen.

http://en.wikipedia.org/wiki/Purified_water
:D
 
http://www.homedepot.com/catalog/pdfImages/3f/3fad4c2b-34e1-4f45-8410-f64dd7feea48.pdf
Phosphoric acid {Orthophosphoric acid} 7664-38-2 CAS # 35.0 -45.0 %
By my calculation it's 38% by specific gravity. (Specific Gravity (Water = 1): 1.25)

http://www.handymath.com/cgi-bin/phostble.cgi?submit=Entry

http://www.finishing.com/512/95.shtml
This is a common problem.

Have you checked your incoming rinse water quality? Tap water can vary from place to place, and it can cause problems. Salts (**chlorine is one) and very high/low pH can accelerate flash rusting. If your tap water is bad, a simple in-line DI system (the cartridge type) can work wonders.

Another solution is to run your final rinse at a slightly acidic pH. Some people will actually use a very small amount of the phosphate concentrate to keep a slightly acidic tank.
Is this a new problem? It looks like your Phosphate concentration is too high and your immersion is too long. Try 2.0 to 2.5 and about a minute to a minute and a half, keep the pH at about 5.5 to 6.0 range and see if that helps. You didn't say whether or not the phosphate stage is heated, if it is keep the temp under 110 degrees. The ppm of the final rinse should be as low as possible, in the less than 50 range.

In order to reduce or prevent flash rusting, it appears to me, you need to use De-ionized water with a 2~2.5% percent concentration of phosphoric acid ( 7~8 oz of prep & etch per gallon of water), keep the rinse solutions temp below 110? F followed by forced air drying the inside of the fuel tank.
 
Last edited:
The forum looks like a treasure trove indeed!
Thank you for sharing.
 
Now all that's needed is to find the best method of rust removal that would preserve as much as what the original metal looked like. (If that's even possible)
 